Material 1.7383
Warmfester Baustahl
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
| HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
|---|---|---|---|---|---|
| 11CrMo910 | ASTM A182F22Class1 | A12CrMo910KG A12CrMo910KW B12CrMo910KG B12CrMo910KW | SCMV4 SFVAF22A SFVAF22B | request |
Material Category: Warmfester Baustahl
Chemical Composition
| C % | Si % | Mn % | P % | S % | Cr % | Cu % | Mo % |
| 0,08 - 0,15 | max 0,50 | 0,40 - 0,80 | max 0,020 | max 0,010 | 2,00 - 2,50 | max 0,30 | 0,90 - 1,10 |
Product Specifications
DIN EN 10216-2 (03/2014)
DIN EN 10222-2 (06/2017)
DIN EN 10273 (10/2016)
Mechanical Properties
| 0,2% Dehngrenze (Rp0,2) | Zeitstandfestigkeit 100.000 h | bei Temperatur |
| >= 235 N/mm² | ~ 300 ° C | |
| >= 225 N/mm² | ~ 350 ° C | |
| >= 215 N/mm² | ~ 400 ° C | |
| >= 205 N/mm² | ~ 221 N/mm² | ~ 450 ° C |
| >= 195 N/mm² | ~ 135 N/mm² | ~ 500 ° C |
| Stabstahl | |||||
| vergütet | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Kerbschlagarbeit (DVM) | Probelage |
| <= 60 mm | >= 310 N/mm² | 520 - 670 N/mm² | >= 18 % | >= 40 Joule | längs |