Material 1.4105
Acero inoxidable
Grade 1.4105 es un acero inoxidable ferrítico. El azufre adicional le da al acero buenas capacidades de corte. Sin embargo, el azufre adicional reduce su resistencia a la corrosión. Con un tratamiento térmico especial, el grado recibe propiedades magnéticas.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
| HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
|---|---|---|---|---|---|
| X6CrMoS17 X4CrMoS18 | AISI 430F UNS S43020 | SUS430F | request |
Material Category: Acero inoxidable
Chemical Composition
| C % | Si % | Mn % | P % | S % | Cr % | Mo % |
| max 0,08 | max 1,50 | max 1,50 | max 0,040 | 0,150 - 0,350 | 16,00 - 18,00 | 0,20 - 0,60 |
Mechanical Properties
| DIN EN 10088-3 (12/2014) Nichtrostende Stähle. Halbzeug, Stäbe, Walzdraht, gezogener Draht, Profile und Blankstahlerzeugnisse aus korrosionsbeständigen Stählen für allgemeine Verwendung. Stäbe | |||||
| geglüht | 0,2% Dehngrenze (Rp0,2) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | bei Temperatur |
| 5 - 10 mm | >= 7 % | ~ 20 ° C | |||
| 10 - 16 mm | >= 310 N/mm² | 500 - 780 N/mm² | >= 7 % | ~ 20 ° C | |
| 16 - 40 mm | >= 250 N/mm² | 430 - 730 N/mm² | >= 12 % | ~ 20 ° C | |
| 40 - 63 mm | >= 250 N/mm² | 430 - 730 N/mm² | >= 12 % | ~ 20 ° C | |
| 63 - 100 mm | >= 250 N/mm² | 430 - 630 N/mm² | >= 20 % | ~ 20 ° C | |
| <= 100 mm | >= 250 N/mm² | 430 - 630 N/mm² | >= 20 % | <= 200 HBW | ~ 20 ° C |
| <= 10 mm | >= 330 N/mm² | 530 - 780 N/mm² | ~ 20 ° C | ||
| >= 230 N/mm² | ~ 100 ° C | ||||
| >= 220 N/mm² | ~ 150 ° C | ||||
| >= 215 N/mm² | ~ 200 ° C | ||||
| >= 210 N/mm² | ~ 250 ° C | ||||
| >= 205 N/mm² | ~ 300 ° C | ||||
| >= 200 N/mm² | ~ 350 ° C | ||||
| >= 195 N/mm² | ~ 400 ° C | ||||
| Draht | |
| kaltgezogen | Zugfestigkeit (Rm) |
| >= 0,05 mm | 500 - 700 N/mm² |
| >= 0,05 mm | 600 - 800 N/mm² |
| >= 0,05 mm | 700 - 900 N/mm² |
| >= 0,05 mm | 800 - 1.000 N/mm² |
| >= 0,05 mm | 900 - 1.100 N/mm² |
| Walzdraht | |
| geglüht | Zugfestigkeit (Rm) |
| <= 100 mm | 430 - 630 N/mm² |
| Gezogener Draht | |||||
| geglüht | 0,2% Dehngrenze (Rp0,2) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | bei Temperatur |
| 0,05 - 0,1 mm | <= 950 N/mm² | >= 10 % | |||
| 0,1 - 0,2 mm | <= 900 N/mm² | >= 15 % | |||
| 0,2 - 0,5 mm | <= 850 N/mm² | >= 15 % | |||
| 0,5 - 1 mm | <= 850 N/mm² | >= 15 % | |||
| 1 - 3 mm | <= 800 N/mm² | >= 15 % | |||
| 3 - 5 mm | <= 750 N/mm² | >= 15 % | |||
| 5 - 16 mm | <= 700 N/mm² | >= 20 % | |||
| <= 100 mm | >= 250 N/mm² | 430 - 630 N/mm² | >= 20 % | <= 200 HBW | ~ 20 ° C |
| >= 230 N/mm² | ~ 100 ° C | ||||
| >= 220 N/mm² | ~ 150 ° C | ||||
| >= 215 N/mm² | ~ 200 ° C | ||||
| >= 210 N/mm² | ~ 250 ° C | ||||
| >= 205 N/mm² | ~ 300 ° C | ||||
| >= 200 N/mm² | ~ 350 ° C | ||||
| >= 195 N/mm² | ~ 400 ° C | ||||
| Profile | |||||
| geglüht | 0,2% Dehngrenze (Rp0,2) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte (HBW) | bei Temperatur |
| <= 100 mm | >= 250 N/mm² | 430 - 630 MPa | >= 20 % | <= 200 HBW | ~ 20 ° C |
| >= 230 N/mm² | ~ 100 ° C | ||||
| >= 220 N/mm² | ~ 150 ° C | ||||
| >= 215 N/mm² | ~ 200 ° C | ||||
| >= 210 N/mm² | ~ 250 ° C | ||||
| >= 205 N/mm² | ~ 300 ° C | ||||
| >= 200 N/mm² | ~ 350 ° C | ||||
| >= 195 N/mm² | ~ 400 ° C | ||||
Material request