Material Category: Stainless steel
Chemical Composition
| C % | Si % | Mn % | P % | S % | Cr % | N % | Ni % | 
| max 0,03 | max 1,00 | max 1,50 | max 0,040 | max 0,015 | 10,50 - 12,50 | max 0,030 | 0,30 - 1,00 | 
Product Specifications
DIN EN 10028-7 (10/2016)
 DIN EN 10088-1 (10/2016)
 DIN EN 10088-2 (10/2016)
 DIN EN 10088-3 (10/2016)
 DIN EN 10088-4 (10/2016)
 DIN EN 10088-5 (10/2016)
 DIN EN 10272 (10/2016)
 DIN EN 10296-2 (10/2016)
 DIN SEW 400 (02/1997)
 DIN 5512-3 (05/2004) zurückgezogen
Mechanical Properties
| DIN EN 10088-3 (12/2014) Nichtrostende Stähle. Halbzeug, Stäbe, Walzdraht, gezogener Draht, Profile und Blankstahlerzeugnisse aus korrosionsbeständigen Stählen für allgemeine Verwendung. | ||||||
| Stabstahl | ||||||
| geglüht | 0,2% Dehngrenze (Rp0,2) bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | Probenlage | bei Temperatur | 
| >= 240 N/mm² | ~ 100 ° C | |||||
| >= 230 N/mm² | ~ 150 ° C | |||||
| >= 220 N/mm² | ~ 200 ° C | |||||
| >= 215 N/mm² | ~ 250 ° C | |||||
| >= 210 N/mm² | ~ 300 ° C | |||||
| <= 100 mm | >= 260 N/mm² | 400 - 630 N/mm² | >= 20 % | <= 200 HBW | längs | ~ 20 ° C | 
| Halbzeug | ||||||
| geglüht | 0,2% Dehngrenze (Rp0,2) bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | Probenlage | bei Temperatur | 
| >= 240 N/mm² | ~ 100 ° C | |||||
| >= 230 N/mm² | ~ 150 ° C | |||||
| >= 220 N/mm² | ~ 200 ° C | |||||
| >= 215 N/mm² | ~ 250 ° C | |||||
| >= 210 N/mm² | ~ 300 ° C | |||||
| <= 100 mm | >= 260 N/mm² | 400 - 630 N/mm² | >= 20 % | <= 200 HBW | längs | ~ 20 ° C | 
| Walzdraht | ||
| geglüht | Zugfestigkeit (Rm) | bei Temperatur | 
| <= 100 mm | 400 - 630 N/mm² | ~ 20 ° C | 
| Gezogener Draht | ||||||
| geglüht | 0,2% Dehngrenze (Rp0,2) bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | Probenlage | bei Temperatur | 
| >= 240 N/mm² | ~ 100 ° C | |||||
| >= 230 N/mm² | ~ 150 ° C | |||||
| >= 220 N/mm² | ~ 200 ° C | |||||
| >= 215 N/mm² | ~ 250 ° C | |||||
| >= 210 N/mm² | ~ 300 ° C | |||||
| <= 100 mm | >= 260 N/mm² | 400 - 630 N/mm² | >= 20 % | <= 200 HBW | längs | ~ 20 ° C | 
| Profile | ||||||
| geglüht | 0,2% Dehngrenze (Rp0,2) bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HBW] | Probenlage | bei Temperatur | 
| >= 240 N/mm² | ~ 100 ° C | |||||
| >= 230 N/mm² | ~ 150 ° C | |||||
| >= 220 N/mm² | ~ 200 ° C | |||||
| >= 215 N/mm² | ~ 250 ° C | |||||
| >= 210 N/mm² | ~ 300 ° C | |||||
| <= 100 mm | >= 260 N/mm² | 400 - 630 N/mm² | >= 20 % | <= 200 HBW | längs | ~ 20 ° C | 
Material request
![[Translate to Englisch:]  [Translate to Englisch:]](/fileadmin/bilder/slider/Werkstoffe/basedo_stahlrohre_werkstoffe.jpg) 
					![[Translate to Englisch:]  [Translate to Englisch:]](/fileadmin/bilder/slider/Werkstoffe/HeaderWerkstoffe.jpg) 
					![[Translate to Englisch:]  [Translate to Englisch:]](/fileadmin/bilder/slider/Werkstoffe/HeaderWerkstoffe2.jpg) 
					![[Translate to Englisch:]  [Translate to Englisch:]](/fileadmin/bilder/slider/Werkstoffe/HeaderWerkstoffe4.jpg)